| Modulus elastis | 20.0 °C | 108.0 - 110.0 GPa | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang, Tabung | |
| 20.0 °C | 108.0 GPa | Anneling | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Tabung Las | |
| 200.0 °C | 96.0 - 97.0 GPa | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang, Tabung | |
| 200.0 °C | 96.0 GPa | Anneling | DIN 17851, VdTÜV WB 230-2, VdTÜV WB 230-1, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Tabung Las | |
| 400.0 °C | 82.0 GPa | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang, Tabung, Tabung Las | |
| Elongasi | 20.0 °C | 16.0 % | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang | Melintang |
| 20.0 °C | 17.0 % | Anneling | DIN 17851, DIN 17864, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17860 | Tabung Las | |
| 20.0 °C | 18.0 % | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang | |
| Kekakalan Brinell | 20.0 °C | 170.0 | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang | |
| Pengurangan luas | 20.0 °C | 30.0 % | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang | Melintang |
| 20.0 °C | 30.0 % | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang | |
| Modulus geser | 20.0 °C | 45.0 GPa | Anneling | DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, VdTÜV WB 230-3, DIN 17862, DIN 17864, DIN 17860 | Tabung Las | |
| Kekuatan tarik | 20.0 °C | 460.0 - 590.0 MPa | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang, Tabung Las | |
| 20.0 °C | 460.0 - 590.0 MPa | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | Pengingatan, Batang | Melintang |
| 20.0 °C | 560.0 MPa | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | | |
| 100.0 °C | 460.0 MPa | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | | |
| 200.0 °C | 340.0 MPa | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | | |
| 300.0 °C | 260.0 MPa | Anneling | DIN 17850, VdTÜV WB 230-3, DIN 17851, VdTÜV WB 230-1, VdTÜV WB 230-2, DIN 17862, DIN 17864, DIN 17860 | | |