DIN 17460 X3CrNiN18-11 Baja Tawar Larutan (+AT) – Grade Suhu Tinggi untuk Tabung Tekanan

Baja suhu tinggi untuk rekayasa tabung tekanan dan boiler uap.

Properti

Umum

PropertiSuhuNilai
Kepadatan20.0 °C7.93 g/cm³

Mekanis

PropertiSuhuNilaiKeterangan
Modulus elastis-100.0 °C206 GPa
20.0 °C196 - 198 GPa
100.0 °C190 - 192 GPa
200.0 °C182 - 183 GPa
300.0 °C174 - 175 GPa
400.0 °C166 - 167 GPa
500.0 °C158 - 159 GPa
600.0 °C150 GPa
700.0 °C142 GPa
800.0 °C134 GPa
900.0 °C127 GPa
1000.0 °C120 GPa
Elongasi20.0 °C30 - 35 %
Rasio Poisson23.0 °C0.3 [-]Typical for Austenitic Stainless Steel
Modulus geser23.0 °C77 GPaTypical for Austenitic Stainless Steel
Kekuatan tarik20.0 °C500 - 700 MPa
Kekuatan leleh Rp0.220.0 °C240 MPa
100.0 °C185 MPa
200.0 °C150 MPa
300.0 °C130 MPa
400.0 °C120 MPa
500.0 °C110 MPa
550.0 °C105 MPa
600.0 °C100 MPa
Kekuatan leleh Rp1.020.0 °C275 MPa
100.0 °C220 MPa
200.0 °C175 MPa
300.0 °C150 MPa
400.0 °C140 MPa
500.0 °C130 MPa
550.0 °C125 MPa
600.0 °C120 MPa

Termal

PropertiSuhuNilaiKeterangan
Koefisien ekspansi termal-100.0 °C1.49E-5 1/K
20.0 °C1.61E-5 1/K
100.0 °C1.63E-5 - 1.67E-5 1/K
200.0 °C1.69E-5 - 1.72E-5 1/K
300.0 °C1.73E-5 - 1.77E-5 1/K
400.0 °C1.78E-5 - 1.81E-5 1/K
500.0 °C1.82E-5 - 1.84E-5 1/K
600.0 °C1.85E-5 - 1.88E-5 1/K
700.0 °C1.87E-5 - 1.91E-5 1/K
800.0 °C1.94E-5 1/K
900.0 °C1.97E-5 1/K
1000.0 °C2E-5 1/K
Suhu operasional maks, jangka panjang0 - 750 °C
Titik leleh1230 - 1480 °CTypical for Austenitic Stainless Steel
Kapasitas panas spesifik-100.0 °C440 J/(kg·K)
20.0 °C450 - 472 J/(kg·K)
100.0 °C487 J/(kg·K)
200.0 °C503 J/(kg·K)
300.0 °C512 J/(kg·K)
400.0 °C520 J/(kg·K)
500.0 °C530 J/(kg·K)
600.0 °C541 J/(kg·K)
700.0 °C551 J/(kg·K)
800.0 °C559 J/(kg·K)
900.0 °C565 J/(kg·K)
1000.0 °C571 J/(kg·K)
Konduktivitas termal20.0 °C14.3 - 17 W/(m·K)
100.0 °C15.8 W/(m·K)
200.0 °C17.5 W/(m·K)
300.0 °C19 W/(m·K)
400.0 °C20.5 W/(m·K)
500.0 °C21.9 W/(m·K)
600.0 °C23.3 W/(m·K)
700.0 °C24.6 W/(m·K)
800.0 °C26 W/(m·K)
900.0 °C27.4 W/(m·K)
1000.0 °C28.8 W/(m·K)
Difusivitas termal20.0 °C3.8 mm²/s
100.0 °C4 mm²/s
200.0 °C4.2 mm²/s
300.0 °C4.6 mm²/s
400.0 °C4.8 mm²/s
500.0 °C4.9 mm²/s
600.0 °C5 mm²/s
700.0 °C5.3 mm²/s
800.0 °C5.6 mm²/s
900.0 °C5.9 mm²/s
1000.0 °C6 mm²/s

Listrik

PropertiSuhuNilai
Resistivitas listrik20.0 °C7.1E-7 Ω·m
100.0 °C7.76E-7 Ω·m
200.0 °C8.49E-7 Ω·m
300.0 °C9.14E-7 Ω·m
400.0 °C9.71E-7 Ω·m
500.0 °C1.02E-6 Ω·m
600.0 °C1.07E-6 Ω·m
700.0 °C1.1E-6 Ω·m
800.0 °C1.14E-6 Ω·m
900.0 °C1.17E-6 Ω·m
1000.0 °C1.19E-6 Ω·m

Properti kimia

PropertiNilai
Carbon0.04 %
Chromium17 - 19 %
Manganese2 %
Molybdenum0.2 - 0.5 %
Nickel9.5 - 11.5 %
Nitrogen0.1 - 0.18 %
Phosphorus0.03 %
Silicon0.75 %
Sulfur0.015 %

Logam

  1. DIN 17744 Grade NiMo23Cr8Fe Alloy Larutan (+AT) – Tahan Karang Superior
  2. NiCr6015 Solution Annealed (+AT) – Ala Konduktor Pemanas Tahan Suhu Tinggi
  3. DIN 17443 X2CrNiMoN18‑15‑4 Solution‑Annealed Stainless Steel – Stainless Steel Bedah Tinggi Performa
  4. DIN 17744 NiCr22Mo7Cu Solution-Annealed Alloy – Ala Tahan Korosi Tinggi & Kelasan Las yang Baik
  5. Baja Karak X2CrNiMoN18-13-3 – Grade DIN 17443, Disolusi Dioles, Ideal untuk Alat Bedah
  6. DIN 17742 NiCr25FeAl3YC Legasi Nikel Disolusi Dioles dengan Perlakuan Penuaan
  7. Leg NiCr7030 DIN 17742 Solution-Annealed: Konduktor Pemanas Berkinerja Tinggi
  8. Baja Stainless Implan DIN 2393-2 X2 CrNiMo 18-15-3 – Premium untuk Instrumen Bedah
  9. DIN 17742 NiCr23Fe: Legasi Tahan Suhu Tinggi dan Korosi
  10. DIN 17744 NiMo28 Lega (+AT) Tahan Korosi untuk Tabung Tekan & Aplikasi Nuklir